Adhesion Testing ③: What Can a Peel Force Curve Tell Us?

💡In This Article

• The relationship between peel strength and the Peel Force Curve
• Why a sawtooth-shaped force curve can indicate Stick-Slip behavior
• How to obtain a more reliable representative peel-strength value

In the previous article, Adhesion Testing ②: Why Do 90° and 180° Peel Tests Give Different Results?, we looked at peel-test configurations and the different failure modes that can appear after peeling. This time I want to push the analysis one step further, into something that’s often overlooked: the shape of the peel force curve.

When we run a peel test, the first number we usually check is peel strength, typically reported in units like N/mm or N/cm. In actual development work, though, I rarely stop at the number alone. Two specimens can both produce an average peel strength of 10 N/cm and still behave completely differently during the test — one might peel smoothly at a relatively constant force, while another repeatedly sticks, releases, and sticks again, producing large force fluctuations. The averages can look similar while the underlying behavior of the adhesive layer is very different. That’s why, in peel testing, the force curve can be just as informative as the final numerical value.


How Is a Peel Force Curve Generated?

During a peel test, the specimen is pulled at a controlled speed while the testing machine continuously records force against displacement or time. The resulting trace is the peel force curve, and the average peel strength is essentially a numerical summary calculated from a selected portion of it. The average value tells us the result; the force curve shows us how that result was produced — which is why, even after checking the average peel strength, an experienced developer will often go back and look at the shape of the curve.

Consider two simplified examples. In Curve A, peel force stays relatively stable as the peel front advances. In Curve B, force repeatedly rises and falls. The two curves could still produce similar average peel-strength values, but they point to very different peeling behavior — a relatively stable curve suggests the peel front is propagating fairly uniformly, while large, repeated fluctuations can indicate local changes in fracture behavior, intermittent debonding and reattachment, or stick-slip behavior. Even when the final number matches, the mechanism behind it can be quite different.


Why Does the Force Curve Sometimes Look Like a Sawtooth?

A perfectly smooth peel-force curve is actually not that common — many adhesive systems produce a small, repetitive sawtooth-like pattern, because the peel front doesn’t always advance smoothly. A simplified stick-slip sequence looks something like this: the adhesive system deforms and stores elastic energy; stress gradually builds around the peel front; once the driving force is sufficient, local crack propagation occurs; the measured peel force drops as the crack advances; the system starts deforming and storing energy again; and the cycle repeats. That produces the characteristic rise-and-drop pattern often associated with stick-slip behavior.

This phenomenon is strongly shaped by the adhesive’s viscoelastic behavior and by how the adhesive interacts with the adherend, and it can also be affected by peel speed, temperature, adhesive thickness, adherend stiffness, surface condition, interfacial adhesion, and adhesive viscoelasticity. A sawtooth curve shouldn’t automatically be read as a defect — it’s better viewed as a clue that the fracture process isn’t proceeding in a completely steady manner.


What Does Stick-Slip Tell Us?

Stick-slip behavior gets particularly interesting during formulation development. Suppose one formulation shows a relatively smooth force curve while another produces large, repetitive force fluctuations — even with similar average peel strengths, the second formulation may have a very different fracture behavior. The fluctuations can mean the crack front keeps getting pinned and then advancing: stick, energy accumulation, local crack advance, slip, reloading, stick again.

The real mechanism in actual adhesive systems can be more complicated than this simplified picture, but the model is useful for understanding why the force curve carries information the average value can’t show. Changes in toughener content, adhesive viscoelasticity, interfacial adhesion, or adherend properties can all alter how the crack propagates — which is one reason I prefer comparing the entire curve when evaluating formulation changes rather than comparing only the average peel strength.


Be Careful With the Initial Peak

Another feature worth attention is the initial peak force. When peeling begins, the system has to transition from a stationary bonded state into steady crack propagation, and during that initial stage, local stress and deformation around the peel front can differ from what happens during steady-state propagation. As a result, the force at the start of the test can sometimes come in higher than the force measured once a stable peel front is established.

That raises a real question: should the initial peak be included when calculating the representative peel strength? The answer depends on the test method and the purpose of the measurement. For a standardized comparison, follow the data-processing procedure the relevant test method specifies. In practical development work, though, it’s often useful to separate the initial transient region from the steady-state peel region — if the goal is comparing steady propagation behavior across formulations, averaging a clearly defined stable portion of the curve gives a more meaningful comparison than letting the initial transient dominate the result. The point isn’t simply “remove the first peak” — it’s defining which portion of the curve represents the behavior you actually want to compare, and applying that rule consistently across all specimens.


The Force Curve Should Be Read Together With the Failure Surface

The force curve becomes far more useful once it’s read alongside the fracture surface. Large fluctuations in force, for instance, can be associated with changes in fracture behavior along the peel path — after the test, one region might show predominantly interfacial failure while another shows cohesive tearing, and a shift like that can help explain why the force curve fluctuates.

That said, a fluctuating curve doesn’t automatically prove adhesive and cohesive failure are alternating. The force signal needs to be read together with the actual fracture surface and the test conditions — an important point in practical analysis. A graph gives us the mechanical response; the fracture surface gives us evidence about where the failure occurred. The two pieces of information become far more powerful together than either one alone.


A Development Note: I Often Looked at the Curve Before the Average

When a peel-test result came back, the average peel strength was naturally the first number I’d check, but I never assumed that two similar averages meant two equivalent results. I’d often open the force curve first and ask whether the overall curve looked similar to the previous formulation, whether the fluctuation had increased, whether the steady-state region was actually stable, whether there was an unusual peak or drop, whether the averaging region was appropriate, and whether the fracture surface supported what the curve seemed to be telling me.

Two formulations might both show 10 N/cm, but if one produces a smooth curve and the other large repeated fluctuations, I wouldn’t treat them as equivalent without digging further — something different is likely happening inside the adhesive layer or at the interface. That’s why I often thought of peel testing not simply as a test that measures a number, but as a test that lets us watch how the adhesive joint actually fails.


Peel Strength Is the Result. The Curve Shows the Process.

Average peel strength is an important metric for comparing adhesive performance, but the process that produces that number lives inside the force curve. Looking at the curve can tell us whether peeling is relatively stable, whether local fracture keeps repeating, whether stick-slip behavior is present, whether the initial transient is unusually large, whether fracture behavior shifts during the test, or whether a formulation change has altered the peeling behavior.

That’s why the habit of looking at both the numerical value and the curve pays off so well in adhesive development — the same principle applies across other characterization techniques too. A DSC result means more once you understand the shape of the thermal transition. A TMA result becomes more meaningful when you look at the dimensional change rather than a single reported value. A DMA result carries far more information than a single Tg number. Peel testing is no different: the number tells us how much force was required; the curve tells us how the joint responded while it was failing.


From Peel Behavior to Formulation Design

Once we understand how an adhesive layer behaves during peeling, the natural next question is what actually controls that behavior. In epoxy adhesives, improving fracture resistance isn’t simply a matter of adding a toughener — the adhesive’s viscoelastic behavior, stress distribution, interfacial adhesion, and its interaction with the adherend can all shape the peeling process.

Beyond tougheners, inorganic fillers are also widely used in epoxy adhesive formulations. Depending on filler type, loading level, particle size, surface treatment, and dispersion state, fillers can influence viscoelastic behavior, stress distribution, modulus, processability, thermal properties, and peel and fracture behavior. Adding filler doesn’t automatically improve every property, of course — as with tougheners, the goal is finding the formulation balance that fits the actual application.

In the next article, Filler Selection in Epoxy Adhesives: More Than Just Filling Space, we’ll look at how fillers affect epoxy adhesive systems and why they’re much more than simple additives used to cut cost or adjust viscosity.

Leave a Reply