Why Doesn’t a Thermally Conductive Adhesive Conduct Heat as Well as You’d Expect? — Electricity vs. Heat: Same Percolation, Different Results

💡 In This Article

  • Why the same percolation produces jumps of completely different size in electricity and in heat
  • The structural limit that keeps thermal conductivity at only a few times that of the resin, no matter how much filler you add
  • How much interfacial thermal resistance weighs, depending on particle size
  • Why bond-line thickness matters more than the thermal conductivity number in real heat dissipation

In an earlier article, What Makes a High-Thermal-Conductivity Filler Different? — Alumina vs. BN vs. AlN, I introduced an S-shaped curve in which thermal conductivity rises sharply once the filler content reaches the percolation threshold. More recently, in the series on conductive adhesives, we saw that resistance falls by several orders of magnitude at the percolation threshold. (See: Why Are Electrically Conductive Adhesives So Sensitive to Thickness?)

Both articles say “it improves sharply once you pass the threshold.” But put the two curves on the same graph, and the size of that “sharply” is completely different. In electricity, resistance changes by hundreds of millions of times or more. In heat, thermal conductivity rises by a few times. This gap is also where the difficulty starts when a customer says, “Can you raise the thermal conductivity just a little?” In this article, we look at why paths built from the same filler give such different results for electricity and heat, and what the difference means for designing a high-thermal-conductivity adhesive.

The Same S-Curve, a Completely Different Scale

Let’s put the two curves side by side.

Electrical and thermal conductivity versus filler content (schematic). Left: electrical conductivity on a log axis, with a jump of 10 or more orders of magnitude at the threshold. Right: thermal conductivity on a linear axis, rising several-fold after the threshold. Plotted together on the same log axis, the thermal conductivity curve looks almost flat.

The resistance curve of a conductive adhesive can only fit on one screen when drawn on a log axis, because it swings by 10 or more orders of magnitude, from insulator level to nearly metal level. The thermal conductivity curve of a high-thermal-conductivity adhesive, by contrast, is drawn on a linear axis. It starts from about 0.2 W/m·K for epoxy resin and, even in highly filled formulations, usually stays at a few W/m·K. The “sharp rise” in the S-curve of the earlier article is a statement on a linear axis, and moved onto the same log axis as electricity it looks more like a gentle slope. Where does the difference come from? From how large the gap is between filler and resin.

FillerResinDifference
Electrical conductivitySilver: about 6 × 10⁷ S/mEpoxy: 10⁻¹² S/m or lessAbout 20 orders of magnitude
Thermal conductivityAlumina: 20–35 W/m·KEpoxy: about 0.2 W/m·KA little over 100 times

For electricity, the resin blocks current almost perfectly. So nothing flows until the particles connect, and the moment even one path opens, current rushes into it. It is a question of “whether it exists or not.” For heat, the resin does not block heat; it only “carries it less well.” Heat still flows through the resin reasonably well even when particles do not connect, and even when they do, that path is not overwhelmingly better. Heat is a question of “how well it conducts,” closer to an average over filler and resin together. That is why the same percolation phenomenon appears over a much smaller range in heat.

However Much You Add — the Resin Is the Bottleneck

Being a question of averages also means that the slowest section decides the whole. For heat to cross the bond line, it has to pass alternately through filler and resin. It moves quickly inside the filler, but slows sharply when it meets the thin resin layer between particles. It is like a highway with unpaved stretches in the middle: however good the highway is, the unpaved stretches decide the total travel time.

A simple calculation confirms this limit. In a classical model (the Maxwell model) that assumes spherical particles scattered evenly and separated from each other in the resin, and a filler whose thermal conductivity is overwhelmingly higher than the resin’s, the thermal conductivity of the composite is approximately:

kcomposite/kresin ≈ (1 + 2φ) / (1 – φ } (φ : filler volume fraction )

Filler Volume Fraction φThermal Conductivity Relative to ResinWith 0.2 W/m·K Epoxy
20 vol%About 1.75×About 0.35 W/m·K
40 vol%About 3×About 0.6 W/m·K
50 vol%About 4×About 0.8 W/m·K

What is surprising in this calculation is that the thermal conductivity of the filler barely appears in the result. Whether the filler is alumina or diamond, as long as the particles are surrounded by resin and kept apart, the thermal conductivity stays at a few times that of the resin. What sets the speed of heat is not the filler but the resin between the particles. Real high-thermal-conductivity adhesives reach higher values than this calculation because, when filler is packed very densely, particles touch each other and paths appear that pass through less resin. The region where the slope increases after the threshold in the S-curve of the earlier article is exactly this regime. That is why a high-thermal-conductivity adhesive requires a much higher volume fraction than a conductive adhesive, and why the fight with viscosity is that much harder.

Wait, What Is 80 wt% Alumina in vol%?

In Part ① of the contact network series, I noted that 80 wt% silver is only about 31 vol%. Alumina, with a density of about 3.95 g/cm³, is far lighter than silver, so the same 80 wt% corresponds to a much higher volume fraction.

(80 / 3.95) ÷ (80 / 3.95 + 20 / 1.2) ≈ 20.3 ÷ 36.9 ≈ 55 vol%

The roughly 55 vol% that I gave in the earlier article as an example of a process limit is right around here. By weight it is the familiar “80%,” but by volume it means a formulation already close to the process limit. And at the same wt%, a lighter filler such as BN (about 2.1 g/cm³) gives a much higher vol%, so when you change fillers, always convert to vol% before comparing.

Interfacial Thermal Resistance Changes the Particle-Size Calculus

In High Thermal Conductivity Adhesives — Why Are They So Difficult to Formulate?, I briefly introduced interfacial thermal resistance between filler and resin, and phonon scattering, as a source of heat loss. This interfacial thermal resistance is also called Kapitza resistance, after the person who discovered it. Here, let’s go one step further and look at what it means for design.

In ceramics and polymers, heat is carried mainly by lattice vibrations, that is, phonons. But a hard ceramic crystal and soft polymer chains vibrate in very different ways. When a vibration in one material tries to pass into the other, a considerable part of it is reflected or scattered at the boundary. It is a little like two people turning a jump rope at different tempos: the rope does not go over smoothly.

Heat flow at the filler–resin interface and the effect of particle size (schematic). Top: phonons are reflected and scattered at the interface, and only part passes through. Bottom: same volume of large versus small particles, where the smaller the particles, the more interfaces the heat has to cross.

What matters is that this resistance accumulates in proportion to interface area. For the same volume of filler, the smaller the particles, the larger the specific surface area, and the more “walls” the heat has to cross on its way through. So in terms of thermal conductivity alone, larger particles are generally the better choice. This is also why formulations that use a lot of fine or nano filler sometimes show lower thermal conductivity than expected.

In Why Does Filler Particle Size Matter?, I said that smaller particles are not always better. That article looked at it from viscosity and dispersion, and for thermal conduction interfacial thermal resistance adds one more reason. But with large particles alone, gaps form and it is hard to raise the packing fraction, so the multimodal particle-size design covered in that article is needed here as well. Large particles reduce the number of interfaces, and small particles reduce the resin layer between large particles. The metaphor from Part ① of the contact network series, “large particles are the main road, small particles are the bridges,” works for heat as it did for electricity. Surface treatment lowers interfacial thermal resistance for the same reason. (See: Silane Coupling Agents ①: How Do Silanes Hold Inorganic and Organic Materials Together?)

The Platelet Filler Trap — in Electricity and in Heat

In the earlier article, I said that because of its platelet structure BN has direction-dependent thermal conductivity and develops orientation during dispensing. This is exactly the same structure as the silver flakes in Part ① of the contact network series. Platelet particles tend to lie flat, parallel to the surface, when applied or pressed. When silver flakes lie down, in-plane electrical conduction is good but the through-thickness direction is at a disadvantage. When BN lies down, in-plane heat flow is good but the through-thickness direction is at a disadvantage. The problem is that, whether the adhesive is connecting electricity or removing heat, the direction you need is in most cases through the thickness. However high the in-plane thermal conductivity of BN, its advantage may not be fully realized in the direction where heat has to go down from the chip to the heat sink. That is why spherical agglomerated BN is used, or platelet BN is mixed with spherical alumina to scatter the orientation. It is also why you should check which direction the thermal conductivity figure in a filler catalog refers to.

Thickness Again

In Part ② of the contact network series, I said that the total resistance of a conductive adhesive is the sum of bulk resistance and interfacial contact resistance, and that plotting resistance against thickness gives a straight line with an intercept. Almost the same equation holds for heat.

Thermal resistance versus bond-line thickness (schematic). An adhesive with higher thermal conductivity but applied thick, versus an adhesive with somewhat lower thermal conductivity applied thin. The two lines cross: on the thin side, the lower-conductivity adhesive has the lower thermal resistance. (BLT: bond-line thickness; k: thermal conductivity of the adhesive; Rinterface: contact thermal resistance between the adhesive and the component or heat sink.)

The practical implication of this equation is large. The performance of a high-thermal-conductivity adhesive is usually compared by thermal conductivity (W/m·K), but what decides how well heat actually gets out of a real part is thermal resistance. As we saw above, doubling the thermal conductivity is very hard. Halving the bond-line thickness, though, halves the bulk thermal resistance on its own. So an adhesive with somewhat lower thermal conductivity that can be applied thinner often gives better heat dissipation in practice.

Here the typical trade-off of high-thermal-conductivity adhesives shows up. To raise thermal conductivity, you need to load large particles at a high level. But a highly filled formulation has high viscosity and does not spread thin, and the size of the largest particle sets the lower limit of the bond-line thickness. The choice made to raise thermal conductivity (k) makes the bond line (BLT) thicker, which raises the thermal resistance again. It is also the same as in the electrical case in Part ② that, as the bond line gets thinner, the interfacial contact thermal resistance takes a bigger share of the total.

When a customer asks, “Can you raise the thermal conductivity just a little?”, what the customer really wants is usually not a higher thermal conductivity number but a lower component temperature. Then raising thermal conductivity may not be the only answer. The same goal can be sought through thickness and interfaces, and that is why you have to look beyond the thermal conductivity number.

Summary

Conductive Adhesive (Electrical)High-Thermal-Conductivity Adhesive (Thermal)
Gap between filler and resinAbout 20 orders of magnitudeA little over 100×
Change at the thresholdA jump of 10+ orders of magnitude on a log axisA several-fold rise on a linear axis
Role of the resinBlocks current almost completelyA bottleneck that carries heat less well
Particle sizeMixing sizes optimizes contactsLarge particles favored by interfacial thermal resistance, but conflict with the thickness limit
Platelet fillersSilver flake orientation → disadvantage through thicknessBN orientation → disadvantage through thickness
Effect of thicknessR ≈ ρ·t/A + 2R<sub>interface</sub>R<sub>th</sub> ≈ BLT/k + 2R<sub>interface</sub>

Final Thoughts

So far in the filler series, from contact networks to high-thermal-conductivity adhesives, we have looked at adhesive performance with the filler at the center. But one bottleneck keeps coming back in these articles: the resin that fills the space between the filler. For electricity it was the wall that blocked current; for heat it was the bottleneck that slowed the flow; and it was also the resin that set the viscosity limit each time we tried to add more filler.

So is that resin all the same resin? We call it “epoxy” in one word, but the epoxy resins a developer actually handles include bisphenol A, bisphenol F, and novolac types, among others, and even among epoxies the viscosity, heat resistance, and handling differ. In the next article, [Why Are There So Many Types of Epoxy Resin? — Bisphenol A, Bisphenol F, and Novolac Compared], we take our eyes off the filler for a moment and look at the base resin itself, the backbone of the adhesive.