💡 In This Article
- The three sources of voids: entrained air, gas generated inside, and space left by shrinkage
- Why some bubbles escape and others stay: a race between viscosity and gelation
- How much gas 1 mg of water can produce during cure
- Why voids collect at interfaces, around fillers, and at edges
- A troubleshooting table for guessing the cause from the shape and location of a void
In the previous article, Silane Coupling Agents ②: Why Doesn’t Adding Silane Help?, I mentioned in passing that excess silane releases alcohol during hydrolysis, and that this alcohol can leave the adhesive during cure and cause voids. Anyone who works with epoxy will meet voids sooner or later. The trouble is that they are hard to see. The surface looks smooth, but a cross-section reveals rows of tiny holes. Initial properties look fine, and the problem only shows up after thermal shock or reflow. And the first question after finding a void is always the same:
“Where did this hole come from?”
In this article, we look at where voids originate, why some bubbles escape while others stay, and why they form in exactly the places they do.
Voids Come from Three Places
Void is a single defect name, but its sources fall into three broad groups.
① Air that was carried in. This is the most common source. Air enters when base and hardener are mixed, when fillers are dispersed, and when the adhesive is dispensed or applied. Air trapped between filler particles or inside agglomerates counts too, as does air left in surface roughness or fine pores on the substrate. The moment the adhesive covers the substrate, the air in those recesses loses its way out.
② Gas generated inside. This is gas newly produced within the material during cure. Absorbed moisture, residual solvent, low-molecular-weight components, and the alcohol released by silane hydrolysis all turn into gas as the material heats up. Moisture held in the substrate, not just the adhesive, can also come out during cure and form voids at the interface.
③ Space left by shrinkage. Voids can form even without any gas. Epoxy shrinks as it cures, and shrinks again as it cools from the cure temperature to room temperature. Where the resin cannot flow in to fill the gap, such as a spot surrounded by material that has already hardened, empty space remains. (See: Why Does Epoxy Shrink as It Cures? — The Origin of Cure Shrinkage and Its Effect on Adhesives)
| Source | Typical Causes | What It Usually Looks Like |
|---|---|---|
| Entrained air | Mixing, dispersion, application, substrate roughness | Round bubbles, fairly uniform in size |
| Gas generated inside | Moisture, solvent, low-molecular-weight species, silane by-products, substrate moisture | Round bubbles that grow during cure or collect at the interface |
| Space left by shrinkage | Cure shrinkage, thermal shrinkage | Irregular shapes, centered in thick sections or at corners |
The distinction matters because the remedies are completely different. For air, look at degassing. For gas, look at drying and control of volatiles. For shrinkage, look at cure conditions and part geometry.

Why Do Some Bubbles Escape and Others Stay?
Not every bubble becomes a void. A bubble that rises to the surface and escapes before cure finishes leaves no trace. The problem is the case where the resin hardens first. The rising speed of a small bubble in a liquid can be estimated with Stokes’ law:

- v: rising speed of the bubble
- r: bubble radius
- Δρ: density difference between the resin and air (about 1,100 kg/m³ for epoxy)
- g: gravitational acceleration
- η: viscosity of the resin
Two things stand out in this equation. The speed is proportional to the square of the radius and inversely proportional to the viscosity. Here is the calculation for a bubble with a radius of 50 µm (0.1 mm in diameter):
| Resin Viscosity | Rising Speed | Time to Rise 1 mm |
|---|---|---|
| 10 Pa·s | About 0.6 µm/s | About 30 minutes |
| 100 Pa·s (a highly filled formulation) | About 0.06 µm/s | About 5 hours |
This is why a highly filled, high-viscosity formulation is hard to degas. For the same bubble size, 10 times the viscosity means 10 times the time to escape. Halve the bubble size and the time quadruples. That is why small bubbles are the ones that stay to the end.
During cure, the situation is more complicated than this calculation. As the temperature rises, viscosity first drops, which makes it easier for bubbles to escape. But as the cure proceeds, viscosity climbs steeply again, and past the gel point, a bubble can no longer move at all. (See: Reading Rheometer Graphs ② — Why Does the Gel Point Matter?)
A void, in the end, is the result of a race between the moment gas appears and the moment the resin sets. Gas formed well before gelation has a chance to escape. Gas formed just before or after gelation is trapped where it is.
What 1 mg of Water Can Do
The most troublesome gas generated inside is water, because the volume difference between liquid water and water vapor is enormous. 18 g (1 mol) of water occupies about 30 L as a gas at 100 °C and 1 atm. Scaled down to 1 mg:
1 mg of water → about 1.7 cm³ of steam (100 °C, 1 atm)
1 mg of liquid water has a volume of about 0.001 cm³. As a gas, it swells by nearly 1,700 times. If 1 g of adhesive holds just 0.1% moisture, and all of it vaporized, the calculation gives a volume of gas larger than the adhesive itself. In reality, the moisture may be dissolved in the resin or only partly vaporized, and the volume depends on pressure. Still, the number shows why “a little moisture” is never a little during cure. Air expands on heating too. A bubble trapped at room temperature (25 °C) grows to about 1.4 times its volume at 150 °C:

A bubble too small to matter grows inside the curing oven, merges with its neighbors, and becomes a visible void. That is why voids that were not visible before cure can seem to “appear” afterward.
A Note on the Assumptions
Both calculations above assume an ideal gas at a constant pressure of 1 atm. Treating water vapor as an ideal gas works better than you might expect. In the steam tables, the specific volume of saturated steam at 100 °C is 1.673 m³/kg, about 1.67 cm³ per mg, only about 2% off from the ideal-gas value (1.70 cm³). Pressure is what changes things. Gas volume is inversely proportional to pressure (PV = nRT), so at 5 atm inside the resin, the same steam occupies one-fifth the volume. More important, the temperature at which water boils itself depends on pressure. At 150 °C, the saturation vapor pressure of water is about 4.7 atm. As long as the pressure in the resin stays above that, the water cannot become gas; it stays dissolved or liquid.
So in a thermocompression process, the dangerous moment is not while the part is under pressure but when the pressure is released. If pressure drops before the resin has gelled, the compressed moisture vaporizes all at once and becomes a void.
Why Do Voids Form Exactly There?
Voids do not appear just anywhere. In a cross-section, you can see where they cluster, and the location tells you the cause.
① The substrate interface. This is the most common location and the most dangerous. Air trapped in surface roughness, and gas from moisture or surface contaminants coming off the substrate, all collect at the interface. If the adhesive does not wet the substrate well, the gap simply becomes a void. An interfacial void directly reduces the bonded area, so it leads straight to lower adhesion and delamination.
② Around the filler. Air trapped in filler agglomerates that does not fully escape during dispersion stays behind as tiny voids around the filler. The same happens when the filler surface is poorly wetted by the resin. The surface-treatment and dispersion problems discussed in the silane articles can show up as voids too. (See: Silane Coupling Agents ①: How Do Silanes Hold Inorganic and Organic Materials Together?)
③ Edges and places where flows meet. In dispensing or filling, air is trapped where the fronts of two flows meet. The same goes for corners and dead ends, where air has no route out.
④ The center of thick sections. Epoxy cure is exothermic. In a thick section, heat cannot escape, so the center gets hotter, more volatiles vaporize, and that region sets first. It can then leave empty space that cannot make up for the shrinkage of the surrounding material.
How Voids Affect Reliability
A few voids often do not lower initial properties much. What makes voids dangerous is that they show up later, in reliability tests.
| Effect | What Happens |
|---|---|
| Stress concentration | Stress collects at the edge of a void, which becomes a starting point for cracks |
| Moisture reservoir | Moisture collects in the void and vaporizes at high temperature, causing delamination |
| Lower thermal conductivity | Air (about 0.026 W/m·K) blocks the flow of heat |
| Lower insulation | Partial discharge can occur inside a void and lead to insulation breakdown |
The second item is especially critical in high-temperature processes such as reflow. When the moisture collected in a void vaporizes in an instant, it expands enormously, as we saw above, and pushes the surroundings apart. This is why delamination occurs far more easily than it would without voids.
Three Principles for Reducing Voids
Just as there are three sources of voids, there are three principles for reducing them.
① Don’t let it in (air). Vacuum degas after mixing and dispersion. Design the dispensing path and application sequence so that air can get out. Pulling too hard a vacuum for too long can boil off low-molecular-weight components or diluents, which can create bubbles instead or change the composition, so find conditions that suit the material.
② Don’t make it (gas). Dry the material and the substrate before use, and control moisture uptake in opened material. Checking the low-temperature weight loss by TGA gives you an advance read on the volatiles a material holds. (See: Reading a TGA Curve: Why Do We Burn a Sample to Weigh It?)
③ Get it out before gelation (time). Use a step cure: hold at a lower temperature, before gelation, long enough for bubbles and volatiles to leave, then raise the temperature to the main cure. In terms of the race we saw above, this delays the moment the resin sets and buys time for the gas to escape.
Diagnosing from Shape and Location: A Void Troubleshooting Table
| Shape and Location of Voids | First Suspect |
|---|---|
| Round bubbles distributed evenly throughout | Air entrained during mixing or application; insufficient degassing |
| Concentrated at the substrate interface | Moisture or contamination on the substrate; poor wetting |
| Size or number increases after cure | Volatiles (moisture, solvent, silane by-products) |
| Irregular shapes, centered in thick sections | Cure shrinkage, cure exotherm |
A Development Note: Voids We Eliminated in Our Process, Voids That Formed in the Customer’s
I mostly worked with one-component adhesives supplied as film, which customers bond by thermocompression. The voids I met in these products were mostly voids that formed during the customer’s own process. At first I could not tell which of the three sources they came from, and looking back, they could have been entrained air or generated gas as well. So I started by eliminating the causes on our side, one at a time. After manufacturing, we degassed for long enough to remove entrained air. The finished adhesive then went through a rest period to let moisture and volatiles out. With the first two sources blocked inside our own process, the adhesive was clean when it shipped. Yet the voids still appeared at the customer.
What remained was the bonding process. Temperature, pressure, time, and heating rate differed a little from one customer to the next, and the differences showed up directly in the amount of voiding. When heated, the viscosity drops, then at some point cure starts and it rises again. If the air and volatiles at the interface cannot escape within that window, they are trapped. The “race between viscosity and gelation” we saw earlier was playing out on the customer’s line.
My conclusion was this. There is a limit to how far you can ask customers to control their process conditions, so the adhesive has to be designed to hold up when conditions drift. Specifically, during bonding the adhesive has to flow enough to push out the air at the interface and fill the surface roughness. The low-viscosity window has to be wide and deep, and gelation has to come after it. So the evaluation shifted from the voids themselves to the flow characteristics: the minimum viscosity, and how wide a window the adhesive stays at that low viscosity. This connects to how we read rheometer graphs. When I face a void, I think the order is to decide first “where does my process end and the customer’s begin,” before deciding where it formed. You have to eliminate the causes in your own process one by one before what is left becomes visible.
Final Thoughts
A void looks like a single hole, but each one carries a story: air that got in, gas that formed, or resin that shrank. Whether the gas got out or was trapped is decided by the race between viscosity and gelation. So when you see a void, ask “When and where did this hole form?” before you ask “How do I get rid of it?” The shape and location usually point to the direction of the answer.
Still, the place where voids gather most often, and most dangerously, was the substrate interface. And besides moisture, there is another invisible culprit behind interfacial voids: a very thin layer of contamination left on the substrate surface. How can a layer that thin and invisible, like release agent, oil, or silicone, undermine adhesion? In the next article, we will look at interface contamination.