Why Do Different Epoxy Resins Behave So Differently? โ€” Reading Epoxy Resins by Their Molecular Structure

๐Ÿ’ก In This Article

  • The differences in molecular structure behind a resin classification table
  • How the length of a single molecule decides liquid versus solid, and the epoxy equivalent weight
  • What two methyl groups leave behind in viscosity and crystallization
  • How the number of functional groups relates to crosslink density and Tg

In an earlier article, Selecting Epoxy Resins and Curing Agents โ€” The Starting Point of Formulation Design, I sorted the main epoxy resins, including bisphenol A, bisphenol F, and novolac types, and summarized which resin and hardener to combine for which use. Bisphenol F has low viscosity and suits high filler loading; novolac has a high Tg but is brittle. Looking at a table like that, questions come up naturally. Why does removing just two methyl groups make viscosity several times lower? Why does a higher functionality raise Tg and make the resin brittle at the same time? Why is one bisphenol A resin a liquid and another a solid?

Through the filler articles, up to [Why Doesn’t a Thermally Conductive Adhesive Conduct Heat as Well as You’d Expect? โ€” Electricity vs. Heat: Same Percolation, Different Results], one thing kept appearing as the bottleneck: the resin filling the space between the particles. This time, we step away from the filler for a moment and look at where the properties of that resin come from in molecular structure. If the earlier article was about “what to choose,” this one is about “why they differ so much.”

Epoxy Resins Share the Same “Hands” but Have Different “Bodies”

The name epoxy resin comes from the epoxy group in the molecule: a triangular ring of two carbons and one oxygen, held under tension, which makes it highly reactive. A curing agent opens this ring and bonds to it, and as molecules link to one another a network forms. That is cure.

Three variables for reading the structure of an epoxy resin (schematic). Epoxy group = the “hands” that react; the backbone in the middle = the “body.” โ‘  Length of the body โ‘ก Shape of the body โ‘ข Number of hands.

Every epoxy resin has the same reacting hands (epoxy groups) and a different body that connects them. And the properties of a resin are largely explained by three variables:

  • Length of the body โ†’ molecular weight, epoxy equivalent weight (EEW), liquid or solid
  • Shape of the body โ†’ viscosity, tendency to crystallize, rigidity
  • Number of hands โ†’ how tight the network is after cure (crosslink density), and Tg

The resins in the classification table of the earlier article are simply different combinations of these three variables. Let’s take them one at a time.

Length of the Body โ€” The Repeat Unit That Separates Liquid from Solid

Bisphenol A epoxy resin is made by reacting bisphenol A with epichlorohydrin. The ratio of the two raw materials sets how many times the bisphenol A unit repeats (the repeat unit, n). A short molecule with almost no repeat units is a viscous liquid like honey. As n increases, the molecule gets longer, viscosity rises, and eventually the resin becomes a solid at room temperature.

Change in bisphenol A resin with repeat unit (n) (schematic). n โ‰ˆ 0: short molecule, liquid, EEW about 180โ€“190 g/eq. As n increases: longer molecule โ†’ higher viscosity โ†’ semi-solid โ†’ solid, EEW several hundred to several thousand g/eq.

This is where the meaning of epoxy equivalent weight (EEW) becomes clear. EEW is “the weight of resin per epoxy group”:

EEW = Molecular weight / Number of epoxy groups per molecule

Whatever its body length, a bisphenol A resin has only two epoxy groups, one at each end. So as the body gets longer, the molecular weight increases while the number of hands stays the same, and the EEW goes up. In the same weight of resin there are fewer hands to react. As a result, the network after cure is looser, and the cured material tends to be more flexible but have a lower Tg.

Another change comes with a longer body. Each repeat unit contains one hydroxyl group (โ€“OH). The longer the body, the more hydroxyl groups, and these form hydrogen bonds with metals and polar surfaces, which contributes to adhesion. This is part of why high-molecular-weight solid epoxies are used in coatings and film-type adhesives.

In practice, you have to remember this relationship. Even among “bisphenol A resins,” different grades have different EEW, and a different EEW means a different hardener ratio. If you change the resin grade and leave the mix ratio as it was, the hardener ends up in excess or short, and the cure fails. (See: When Epoxy Doesn’t Cure Fully, Where Should You Start Looking? โ€” The Four Types of Incomplete Cure)

Shape of the Body โ€” What Two Methyl Groups Leave Behind

The difference between bisphenol A and bisphenol F lies in the central carbon that links the two benzene rings. In the A type, this carbon carries two methyl groups (โ€“CHโ‚ƒ); in the F type, it carries hydrogen in their place. It is a very small difference for the molecule as a whole, but it leaves a quite distinct mark on the properties of the resin.

Comparison of the central carbon in bisphenol A and F types (schematic). A type: two methyl groups โ†’ bulky, restricted rotation. F type: two hydrogens โ†’ small, free rotation.

โ‘  Viscosity. Methyl groups are bulkier than you might think. With two methyl groups on the central carbon, the two benzene rings cannot rotate freely, and the molecule becomes stiffer and larger. Such molecules have difficulty sliding past one another, so viscosity is high. With the methyl groups replaced by hydrogen, the F type is smaller and more flexible, and the molecules slide past each other more easily. That is why, among standard liquid grades, the viscosity of the F type is only a fraction of that of the A type.

โ‘ก Rigidity of the cured material. After cure, the same reason works the other way. The A-type body, with its restricted rotation, holds the chains firmly even after cure, so in general the cured A type has a Tg equal to or slightly higher than the F type. The advantage of low viscosity in the F type and its slight deficit in heat resistance are two sides of one coin, coming from the same structural cause.

โ‘ข Crystallization. When a molecule is symmetric and of high purity, molecules can line up in an orderly way at low temperature and form crystals. This is why a high-purity liquid bisphenol A resin turns cloudy and solid after long storage in the cold. The statement in the earlier article that biphenyl epoxies are crystalline is in the same vein: the flatter and more symmetric the body, the more easily molecules stack up. Interestingly, mixing A and F types makes crystallization less likely, because molecules of different shapes interfere with each other’s lining up. I will cover this crystallization in detail in the next article.

Number of Hands โ€” What Happens When the Network Gets Tight

If bisphenol resins are bifunctional, with two hands, novolac resins are multifunctional, with several hands on one molecule. The number of hands directly affects the network structure after cure.

Comparison of cured networks by functionality (schematic). Bifunctional: chains run long, with large distances between junctions. Multifunctional: bonds extend from one molecule in many directions, with short distances between junctions.

It is easiest to think of how tight a network is as the distance between crosslink points. Molecules with two hands link up like a chain and branch only occasionally, so long chains sit between crosslink points. A molecule with many hands bonds in several directions within a single molecule, so the chains between crosslink points are short. That is what a high crosslink density means. When the chains between crosslink points are short, the chains have less room to move. Tg is the temperature at which chains begin to wriggle, so the more tightly they are tied, the higher the temperature has to be before they can move, and Tg rises as a result. This is the structural reason novolac resins are used for high heat resistance.

For the same reason, though, there is a price to pay.

โ‘  Brittleness. If chains have no room to move, external impact or deformation cannot be absorbed by chain motion. With nowhere for the energy to go, it turns into cracks, and the cured material is hard but breaks easily.

โ‘ก High viscosity. A molecule with many hands is usually large and has many benzene rings, so it often has high viscosity even before cure, or is a solid at room temperature.

โ‘ข Hard to cure fully. This is easy to overlook. The higher the Tg of a resin, the faster its Tg rises as cure proceeds, and when Tg reaches the cure temperature, the molecules freeze and the reaction effectively stops. This is vitrification. To cure a high-Tg resin fully, you therefore need a higher cure temperature or a post-cure. If you keep the cure temperature as it is and just add more novolac, you may not get the expected Tg and may end up with an undercured material.

That’s Why Resins Are Blended

Summing up so far, the properties of an epoxy resin are built so that gaining one means losing another. Make the body lighter to lower viscosity, and rigidity falls. Add hands to raise Tg, and it gets brittle and harder to cure. Lengthen the body and it becomes more flexible but Tg drops. So in real development, instead of meeting every requirement with one resin, resins of different structures are blended to strike a balance. Take bisphenol A as the base, add F type if you need lower viscosity, add novolac if you need heat resistance, and make up for the resulting brittleness with a toughener. The “combination guide by application” in the earlier article can be seen as organizing exactly where that balance is struck.

Summary

Structural VariableWhat ChangesWhat You GainWhat You Lose
Longer body (n increases)Molecular weight and EEW rise; more hydroxyl groupsFlexibility, adhesion, solid formLower crosslink density and Tg; higher viscosity
Methyl groups removed (A โ†’ F type)Smaller molecular volume; more freedom to rotateLow viscosity, high filler loadingSome rigidity and Tg
Symmetric, high-purity bodyOrderly arrangement of molecules(For crystalline resins) low moisture absorption, low CTELow-temperature crystallization
More hands (multifunctional)Shorter distance between crosslink pointsHigh Tg, heat resistance, chemical resistanceBrittleness, high viscosity, hard to cure

A Development Note: Not All “Heat Resistance” Is the Same

I once had to raise the heat resistance of an adhesive so that it could survive a test with a short exposure to high temperature. When someone says “let’s raise the heat resistance,” nearly every time, the first thought is to raise Tg. I thought so too, at first. When I asked epoxy resin suppliers for ways to improve it, it was the same: most came back with a novolac resin to raise Tg.

But the heat resistance required then was not the kind that Tg explains. In the field, the single word “heat resistance” is used in more different senses than you might expect. In some cases Tg matters; in others it is the temperature at which the resin starts to decompose; in yet others it is how much adhesion is retained at high temperature. To solve the problem properly, I first had to work out “which kind of heat resistance.” Looking back, the “heat resistance” a developer meets can be roughly divided as follows.

CategoryWhat It Looks AtWhen It Is Mostly a Problem
Glass transition temperature (Tg)Temperature at which the resin changes from hard to softWhen stiffness and dimensional stability must be maintained at the service temperature
Decomposition temperature (Td)Temperature at which the resin decomposes and starts to lose weightWhen the part passes through a momentary very high temperature
High-temperature adhesionBond strength measured at elevated temperatureWhen load or peel stress is applied while hot
Long-term heat agingRetention of properties after long exposure to high temperatureWhen used at high temperature for thousands of hours or more (discoloration, embrittlement)
Heat resistance after moisture absorptionBehavior when passing through high temperature while holding moistureWhen absorbed moisture vaporizes suddenly and causes lifting or delamination
Thermal expansion (CTE)How much it expands above and below TgWhen the difference in expansion from the substrate builds stress at the interface

Tg is only one of these items. Raising Tg with a novolac resin can increase brittleness and may even work against high-temperature adhesion or thermal shock. Conversely, if heat resistance after moisture absorption is the problem, the moisture uptake of the resin and control of volatiles are a more important key than Tg. (See: Why Do Voids Form in Epoxy? โ€” Where Voids Come From and Where They Stay)

When asked to “raise the heat resistance,” I think the better habit is to find out first in which test and in what way the heat resistance failed, before changing the resin. That habit saves a lot of trial and error afterward.

Final Thoughts

In this article, we saw that epoxy resins share the same reacting hands but have different bodies, and that the length and shape of the body and the number of hands change viscosity, Tg, and even how hard the resin is to cure. But one thing passed by quickly in the section “Shape of the Body โ€” What Two Methyl Groups Leave Behind”: a high-purity liquid resin turning cloudy and solid in the cold. That is crystallization.

The first time you see a resin you have been using happen to be solid in its drum one winter day, or white granules settled at the bottom, it is easy to be alarmed. Has the resin gone bad? Has it started to cure? Is it all right to use as it is? And why does it happen more readily to a resin of higher purity?

In the next article, Why Does Liquid Epoxy Solidify in Winter? โ€” Resin Crystallization, we will look at what this phenomenon, solidifying without curing, really is, and how to tell it apart and handle it in the field.

Leave a Reply